Tungsten Granule Dosage
Tungsten granule is oxidized under oxygen atmosphere at 650℃ and releasing 195.85 Kcal /mol. Therefore, the sample will be heated to high temperature quickly and oxidized to CO2 and SO2.
The testing result is changed with tungsten granule dosage, following is a table to show the different testing result by using 0.5kg sample and 0.5g, 1.5g, 2.0g, and 2.5g flux.
Flux(g) | 0.5 | 1.0 | 1.5 | 2.0 | 2.5 | ||||||
Content | C | S | C | S | C | S | C | S | C | S | |
A | 1 | .62 | 0.037 | 0.62 | 0.037 | 0.62 | 00.037 | 0.62 | 0.037 | 0.62 | 0.037 |
2 | 0.590 | 0.0316 | 0.618 | 0.0366 | 0.614 | 0.0355 | 0.612 | 0.0345 | 0.617 | 0.0345 | |
3 | 0.52 | 2.54 | 0.25 | 0.41 | 0.28 | 1.00 | 0.69 | 1.34 | 0.65 | 0.25 | |
B | 1 | 4.00 | 0.026 | 4.00 | 0.028 | 4.00 | 0.028 | 4.00 | 0.028 | 4.00 | 0.028 |
2 | 3.60 | 0.024 | 3.98 | 0.028 | 3.97 | 0.031 | 3.98 | 0.028 | 3.98 | 0.028 | |
3 | 0.57 | 13.76 | 0 | 1.83 | 0.15 | 1.56 | 0.25 | 1.56 | 0.15 | 2.09 | |
C | 1 | 4.88 | 4.88 | 4.88 | 4.88 | 4.88 | |||||
2 | 4.10 | <0.04 | 4.86 | 0.053 | 4.88 | 0.054 | 4.88 | 0.056 | 4.89 | 0.054 | |
3 | 0.51 | 64 | 0.35 | 1.64 | 0.12 | 1.65 | 0.12 | 1.23 | 0.54 | 0.86 |
Note:
A: Carbon steel
B: Pig iron
C: High carbon ferrochrome
1: Standard value (%)
2: Test value (n=5) (%)
3: Differnece (%)
Therefore, the quantity selection is an important process for testing C and S value.
If you have got any interest in tungsten granule, please feel free to contact Chinatungsten.